Magnetic,thermal stability and dynamic mechanical properties of beta isotactic polypropylene/natural rubber blends reinforced by NiZn ferrite nanoparticles
2020-01-07LihJiunYuShrimHjAhmIngKongMouTrwnhShmsulBhriBinRzkElngoNtrjnChunKitAng
Lih-Jiun Yu ,Shrim Hj Ahm ,Ing Kong ,Mou A.Trwnh ,Shmsul Bhri Bin A Rzk ,Elngo Ntrjn ,Chun Kit Ang
a Department of Mechanical Engineering,Faculty of Engineering,Technology and Built Environment,UCSI University,No 1,Jalan Menara Gading,UCSI Heights(Taman Connaught),Cheras,56000,Kuala Lumpur,Malaysia
b School of Applied Physics,Faculty of Science and Technology,University Kebangsaan Malaysia,43600,Bangi,Selangor Darul Ehsan,Malaysia
c School of Engineering and Mathematical Sciences,La Trobe University,Bundoora,VIC,3086,Australia
d Department of Physics,College of Science,Al-Hussein Bin Talal University,P.O Box 20,Ma'an,Jordan
e Department of Food Science and Technology,University Malaysia Terengganu,Kuala Nerus,Terengganu,Malaysia
ABSTRACT The dispersion of magnetic nanoparticles in matrix is crucial to ensure optimum performance of the composite.The difficulty level of achieving good dispersion is further increase when a multi-phases of matrix is present.A pre-coating technique of magnetic nanoparticles with polypropylene using ball-mill prior to melt-blending process was employed to prepare a multi-phases thermoplastic natural rubber composite.The effect of filler loading(2 wt%-10 wt%)on morphology,structure,magnetic properties,thermal stability and dynamic mechanical properties of the composites were investigated.It was found that the NiZn ferrite nanoparticles act as nucleating agent to form beta isostatic polypropylene thermoplastic composites.The composites'magnetic properties are directly dependent on the filler concentration.The dispersion of magnetic fillers in polymer matrix plays role in affecting the magnetic properties and thermal stability.The preference of filler to locate at amorphous phase has distorted the chain orientation of natural rubber and polypropylene.Hence,the polymorphism and crystallinity of the matrix varied as the filler loading increased,affecting the dynamic mechanical properties.It was found that 8 wt%NiZn nanocomposite exhibits highest E’and tanδ,indicating the dynamic mechanical properties of NiZn nanocomposite are affected by β-phase degree.
Keywords:Magnetic Thermoplastic natural rubber Nanoparticles Composites
1. Introduction
Thermoplastic natural rubber(TPNR)is an analogue of the thermoplastic elastomers(TPE).They are prepared by blending rubber with thermoplastics such as polyolefins,offering an intermediate properties between these two polymers.According to Ibrahim&Dahlan[1],the TPNR exhibits improved impact strength,ductility and stiffness,as compared to the rubber and polyolefins.In addition,the ease of processing and high recycling ability are the main advantages of the TPE.Various fillers were incorporated into the thermoplastic elastomer matrices,aimed to achieve desired properties in the specific application.However,there is a need for proper mixing between the fillers and TPNR matrix in order to achieve optimal results.
Incorporation of ferrite nanoparticles in polymeric matrix has offered superior performance in microwave absorption[2-6]and information storage[7-9],potentially applicable in stealth technology [10] and energy storage. The ferrite nanoparticles are embedded in polymeric matrix,enhancing the magnetic properties and mechanical properties of the polymers[1,11-13].These composite materials offer advantages,in term of flexibility of shaping,cost saving and reducing environmental attack on the filler counterparts.However,a good dispersion of the magnetic fillers in polymer matrix is hard to achieve,magnetic particles have higher tendency to form agglomerate due to their magnetic interaction.Furthermore,the control of fillers dispersion could be tougher,especially when the fillers are incorporated into multiple phase's matrix.Premphet&Horanont[14]observed that the phase structure of the ternary phase composite can be either exhibits as a separate dispersion of the phases or encapsulation of the fillers by elastomer.These two phase structure showed different crystallization behavior and dynamic mechanical properties,depends on the polarity of the elastomer.
Numerous studies emphasized on the preparation and characterization of β isostatic polypropylene[15-19].The formation of β isostatic polypropylene with the presence of nucleating agent in multiple phase thermoplastic blends and their properties are remained unclear.In this paper,the work focused on the relationship between the microstructure and the properties of the NiZn ferrite loading in binary phase matrix which consists of natural rubber and polypropylene.The effect of filler loading on magnetic properties,thermal stability and dynamic mechanical properties of the nanocomposites were studied.
2. Materials and methods
Nickel zinc ferrite nanoparticles(Ni0.5Zn0.5Fe2O4),with 98.5%purity,average particle size 10-30 nm,were obtained from commercial suppliers in powder form.Natural Rubber(NR)and polypropylene(PP)were supplied by the Rubber Research Institute of Malaysia(RRIM)and Mobile(M)Sdn.Bhd.Liquid natural rubber(LNR)was prepared by photosynthesized degradation of NR in visible light.
The TPNR was prepared from PP,NR and LNR with a weight ratio of 70:20:10.LNR was used as the compatibilizer in the mixture.NiZnFe2O4nanopowder was ball milled with PP for 15min prior incorporated in the TPNR matrix by melt blending techniques in the laboratory.In this study,the TPNR/NiZnFe2O4nanocomposite with 2 wt%-10 wt%NiZnFe2O4was prepared using Thermo Haake at rotation speed of 100r⋅min-1,180°C,for 13min.After the blend,the samples were hot-pressed into a thin sheet of 1 mm in thickness using a hydraulic press at 185°C.Field emission scanning electron microscopy(FESEM)graph for the nanocomposite was obtained from a fractured surface.Transmission electron microscopy(TEM)graph for the nanocomposite was obtained by Phillips CM-12.Microstructure studies on nanocomposites were carried out by Xray diffraction (XRD; Siemens D5000) with CuKα1radiation(λ=1.5406 Å).Magnetization measurements were carried out using a vibrating sample magnetometer,VSM(Model 7404),to obtain the M-H loop at room temperature(25°C).Thermogravemetric analysis and dynamic mechanical analysis were carried out using TGA 50(Shimadzu)and DMA 2980(TA instrument)respectively.
3. Results
3.1. Magnetic properties
The hysteresis of pure NiZn nanoparticles and nanocomposites with different filler content was measured at room temperature.Fig.1 exhibits the loops for the six samples with 2 wt%,4 wt%,6 wt%,8 wt%,10 wt%and 100 wt%of NiZn ferrite.The corresponding results from VSM for all samples are listed in Table 1.Initial susceptibility and permeability of the nanocomposite were obtained from the initial magnetization curve from VSM and listed in Table 1.As the filler content increased,the values of saturation magnetization(MS),remanence(MR),initial susceptibility(χi),and initial permeability(μi)increased,except for coercivity(Hci).The results are consistent with previous reports on other magnetic polymer by Kong et al.[2]and Gokturk et al.[20].For all nanocomposites,it is observed that the initial permeability is lower than 100 wt%NiZn ferrite.This is because the ferrite grains are embedded in the TPNR matrix.Vijutha Sunny[13]suggests that the nonmagnetic rubber matrix causes a discontinuity in the nanocomposite giving way to a demagnetizing field,thus,reducing the permeability at lower filler contents.
Fig.1.M-H hysteresis loop obtained from the samples with various filler loading.
Table 1Corresponding results obtained from VSM.
The results indicate that saturation magnetization and remanence are increasing whereas the intrinsic coercive force value show a slightly decreasing,ranging from 22.06 to 20.35Oe.The Hcivalues of the nanocomposite are close to theHcivalue of 100 wt%of NiZn ferrite(20.35Oe).The values are different from those previously reported by Ramajo et al.[21]and Yang et al.[22],as theHcivalues of magnetic composites are almost constant and independent to the filler loading.It is known that the coercive force of a material is sensitive to the microstructure,related to the anisotropy of the magnetic particle.A good mixing process enables the magnetic particles to be randomly orientated and dispersed uniformly in the polymer matrix.The magnetic particles are isolated from each other in the polymer matrix.This could reduce the agglomeration of the magnetic particles,giving a higher mean distance between the particles.As the mean interparticle distance increases,the magnetic interaction between the ferrite particles decreases.The TPNR matrix restricts the alignment of the magnetic moment of the ferrite.Therefore,it is hard to demagnetize the ferrite particles with higher mean distance between the particles,thus the coercive force is high in the lower ferrite loading in the composite.Fig.2 shows SEM micrograph of the fractural surface of 2 wt%and 10 wt% of NiZn ferrite nanocomposite. The white spheres embedded in the TPNR matrix are NiZn ferrite nanoparticles.The NiZn ferrite particles in 10 wt%nanocomposites have a higher tendency to agglomerate into larger size,leaving a large interparticle distance between the nanoparticles while NiZn ferrite particles in 2 wt%nanocomposites are closed and isolated by the matrix.
Application of a field H causes the magnetic induction to increase in the field direction.Magnetization reaches saturation when all the magnetic dipoles within the materials are aligned in the direction of the magnetic field.The saturation magnetization is only dependent only on the magnitude of the atomic magnetic momentsmand the number of atoms per unit volumen,MS=nm.Saturation magnetization is also commonly expressed as the magnetic moment per mass.This specific saturation magnetization is linearly dependent on the mass fraction of ferrite and obeys the general relation:MS=MfWf.WhereMfandWfare the saturation magnetization and weight fraction of the ferrite,respectively.The saturation magnetization of the nanocomposite depends on the content of the filler with magnetic moments in a given mass fraction.The experimentalMSvalue and the theoreticalMSvalue were plotted in Fig.3.The results indicate good agreement,as both experimental and theoreticalMSvalues are similar.
3.2. Crystallography structure
Fig.2.FESEM micrograph of(a)2 wt%NiZn ferrite nanocomposite(b)10 wt%NiZn ferrite nanocomposite.
Fig.3.Comparison of theoretical and experimental Ms values.
Fig.4.X-ray diffractograms of the nanocomposites with different filler content.
The X-ray diffractograms of the TPNR and nanocomposites with various filler loadings are shown in Fig.4.The figure illustrates that two phases,crystalline phase and amorphous phase co-exist in both the TPNR and the nanocomposites.For all samples,the semiamorphous phases of the TPNR appear at the lower 2θ degree(<30°)and 42.48°.According to Alariqi et al.[23],the sharp peaks(14.05°,16.9°,18.5°,21.8°)in this range contributed by the crystallinity of the α-phase isotactic PP.Meanwhile,the broadening of the amorphous region of NR could be seen clearly in the X-ray diffractogram of TPNR.Tang et al.[24],Wang et al.[25]and Jancar[26]agreed that the thermodynamically stable β-phase formation of polymorphic PP is hard to achieve under normal processing condition.Varga et al.[27]and Horvath et al.[28]stated that the βphase can be obtained when the PP undergoes isothermal crystallization process, high shear field crystallization process or blended with β-phase nucleating ability polymer.It can be seen that the β-phase PP which located at 16°appears when NiZn ferrite incorporated in the TPNR.The proportional increment of the intensities β-phase with the filler content under constant processing condition,has demonstrated that the ability of NiZn ferrite to act as a nucleating agent,to promote β-phase formation of PP.The highest relative content of β-phase PP were obtained at 8 wt%NiZn ferrite,then reduced 25%at 10 wt%NiZn ferrite.The tendency of NiZn ferrite particle to form agglomerates at high filler content has weakened the nanoscale confinement structure formation,resulted disoriented PP crystals formation,hence led to an overall reduction in crystallinity of PP. The characteristic peaks of NiZn ferrite matched with the database(JCPDS file no.00-008-0234)to confirm the planes of NiZn ferrite in the nanocomposites.There is no structural change NiZn ferrite after incorporating in the TPNR,because the peak position of the NiZn ferrite peaks remain unchanged.It can be seen that,the increment of NiZn ferrite loading leads to the increment of the intensity of the characteristic peaks for NiZn ferrite,significantly at the major intensity peak at plane(311).By referring to the NiZn ferrite peaks in plane(311),the fractional crystallinity of the nanocomposites are 0.51,0.52,0.54,0.62,0.87 for 2 wt%-10 wt%nanocomposites respectively.Diffraction peaks and the amorphous phase of TPNR reduced at higher filler content since the characteristic peaks of crystalline NiZn ferrite became dominant.This result is consistent with Sun et al.[11]and Low et al.[29].The crystallinity and amorphous region of TPNR were suppressed after introducing fine NiZn ferrite particles into the system,due to the migration of fine particles interfering the preferred orientation of the TPNR.The magnetic dipole interaction of NiZn ferrite is higher in the low crystalline matrix because of the higher freedom of spin rotation at the amorphous phase,hence,leading to better magnetization properties NiZn ferrite in TPNR.At higher filler loadings,more NiZn ferrite particles located in the amorphous phase.Therefore,less external force(Hci)is required to orientate spin according to the applied field.
Fig.5 illustrates the TEM micrograph of the NiZn ferrite nanocomposite.The dark spheres are NiZn ferrite particles,the grey regions are the NR phase,and the white regions are the PP phase.The phase structure of the NiZn ferrite nanocomposites shown in Fig.5 is the combination of the two types of phase structure,which observed by Premphet&Horanont[14].It can be seen that the NiZn ferrite particles are distributed homogenously in both the NR and PP phase,while some aggregation of the NiZn ferrite particles is likely to occur in the NR phase,due to the slightly high viscosity of NR,which limits the dispersion of NiZn ferrite particles during the mixing process.According to Osawa et al.[30],the movement of polymer segment surrounded the filler was limited by polymerparticle interaction.Hence,the preference of NiZn ferrite particles to aggregate in NR phases leads to the rapid drop of crystallinity of the TPNR phase.Based on the morphology examination,a schematic diagram was drawn to show the phase structure of the NiZn ferrite nanocomposite.Fig.6(a)shows the arrangement of TPNR molecule chains which consist of semi-crystalline phase and amorphous phase.After incorporated with NiZn ferrite with higher electronegative attraction,the molecule chain of TPNR was distorted by the NiZn ferrite particles with higher electronegative attraction and hence,affected the TPNR crystallography structural,as shown in Fig.6(b).
Fig.5.TEM micrograph of 2 wt%NiZn ferrite nanocomposite.
Fig.6.Schematic diagram of the arrangement of the TPNR molecule chains(a)before incorporated with NiZn ferrite(b)after incorporated with NiZn ferrite.
3.3. Thermal properties
Fig.7.Thermogram of NiZn ferrite nanocomposite.
Table 2Data obtained from thermogram graph.
The thermal stability of the NiZn ferrite nanocomposite was studied by thermogravity analysis under the nitrogen flow to prevent unwanted weight addition of oxidized product during heating process and was illustrated in Fig.7.The corresponding data obtained from thermogram are listed in Table 2.It was found that the thermal degradation of TPNR and its nanocomposites takes place through a two-step process,remarkable at decomposition temperature around 360°C and 440°C. The first decomposition temperature was due to the decomposition of the NR phases while the latter was due to the decomposition of the PP phases.The difference of crystallinity degree of these two phases impacts to the decomposition temperature,whereas the lower crystallinity phase(NR)provided more free volume to enable the molecules movement during heating process.The NiZn ferrite has higher resistance to the thermal degradation because the molecules are highly crystalline oriented.The thermal decomposition temperature of NR phases and PP phases of the NiZn ferrite nanocomposites were studied at the 10%weight loss and 50%weight loss of samples,denoted byT10andT50respectively in Table 2.The results revealed that theT10andT50are slightly shifted to the higher value.It is clear that the addition of NiZn ferrite leads to an increase of the TPNR thermal stability.Similar thermal stability behavior of the addition ferrite has been reported by Cha&Kim(2007)[31]and Puryanti et al.(2007)[32].The delaying of volatile products diffuse from bulk polymer was attributed to the physical absorption between the NiZn ferrite surface and their surrounding TPNR molecule chains.The increment of NiZn ferrite content provided more absorption interaction with the TPNR molecules,hence retarded the decomposition process of both NR phases and PP phases.The endset temperature of the nanocomposite was denoted byTT.Apparently,the values ofTTare inversely proportionally to the NiZn ferrite content,due to more heat energy are required to decompose large quantity of hydrocarbon compounds that presence in the samples.The residual weight percent demonstrated the remaining carbonyl products and NiZn ferrite which are incombustible at 500°C.These residual weight percent approached the initial filler weight percent,indicating a homogeneity blends were achieved by the blending of NiZn ferrite into the TPNR matrix.
3.4. Dynamic mechanical properties
The temperature dependence of storage modulus (E') of different filler loading of NiZn ferrite nanocomposite were studied at the fixed frequency of 1 Hz.From Fig.8(a),the NiZn ferrite addition had induced a higherE'value at-80°C.The large particle surface of nanosized NiZn ferrite tends to increase the stiffness of the TPNR in glassy state.Diez-Pascual et al.[33]explained the increment ofE'value is attributed to the effective load transfer from the polymer matrices to the fillers, resulting from the good dispersion of fillers in the matrix.TheE'value of 2 wt%NiZn ferrite showed a drastic drop at-73°C and exhibited lowestE'values above its glass transition temperature;this result is in agreement with Varga et al.[27]findings,the formation of β-phase PP reduced the tensile strength of nanocomposite,provided higher impact strength and ductility in contrast.However,as NiZn ferrite loading increases,the β-phase's toughening effect was overtaken by the reinforcement effect of the NiZn ferrite nanoparticle.HighestE'was achieved by 8 wt%NiZn ferrite,further increment of NiZn ferrite loading was found ineffective in load transfer.The reduction ofE'at 10 wt%possible due to reduction in β-phase PP and agglomeration of NiZn ferrite nanoparticles.
Fig.8.(a)Storage modulus of nanocomposites with various filler loading(b)tanδ of nanocomposite with various filler loading.
From Fig.8(b),tanδ peak value of all nanocomposites is higher than the corresponding tanδ peak value of TPNR.The increasing trend of the tanδ peak values was contributed by the hysteresis loss upon dynamic tensile stress.This is probably due to the particleparticle friction and particle-matrix interface interaction when more filler were introduced to the TPNR matrix.The particle-matrix interface interaction due to the presence of β-phase around the NiZn ferrite particle resulted increasing in the damping characteristic of the nanocomposites.Similar increment of tanδ peak value was observed by Weon&Sue[34]in the CaCo3/high crystalline PP system with the presence of β-phase.The corresponding glass transition temperatures(Tg)of the TPNR and the NiZn nanocomposites were identified from the tanδ peak position.It can be seen that there are two glass transition temperatures as shown by TPNR and NiZn nanocomposites. The firstTg(approximately-70°C)is theTgfor NR,while the latter glass transition temperature approximately located at 11°C is theTgfor PP in the TPNR system.The results shows the bothTgvalues had shifted to the lower value after incorporated with the NiZn ferrite particles.This implies that the incorporation of fillers in the TPNR matrix induced β-phase formation,led to an increment in the free volume of the polymer chain, thus promotes the molecular mobility at lower temperature.It can be observed that both glass transition temperatures(NR and PP)of 8 wt%NiZn nanocomposite is relatively low(approximately-73°C and 4°C).This is corresponding to high degree of β-phase presents in 8 wt% NiZn nanocomposite,resulting in more molecular chains mobility.The loss of energy attributed to the lower cohesive force by the β-phase,leads to easier slipping on the lamella chains when the degree of βphase increased[35].
4. Conclusions
Thermoplastic natural rubber exhibits as a non-magnetic material. The magnetic properties of TPNR can be improved by incorporating magnetic particles.It was found that the magnetic properties of the nanocomposites improved as the ferrite loading increased.The saturation magnetization of the nanocomposites can be estimated by its weight fraction of filler loading,following linear proportion of filler magnetization and its weight fraction relationship.The reduction of crystallinity of TPNR leads to higher magnetization properties due to the higher degree of spin rotation of the NiZn ferrite particles available in the amorphous phases.NiZn ferrite was found to act as a β-phase nucleating agent in the ternary phase composite,with the aids of pre-coating technique.The thermal stability,stiffness and softening point of the thermoplastic natural rubber were enhanced with the NiZn ferrite addition.It was found that 8 wt%NiZn nanocomposite exhibits highestE’and tanδ,indicating that the dynamic mechanical properties of NiZn nanocomposite are improved with increment of β-phase degree.
The scope of this work was limited to a fixed ternary phase blend ratio of PP:NR:LNR.The work could be extended to investigate effect of beta isotactic polypropylene formation when different ratio of ternary blend is applied.
Conflicts of interest
The authors declare no conflict of interest.
Acknowledgments
The authors would like to thank the support from the National Science Fund(NSF),MOSTI,UKM and UCSI.
杂志排行
Defence Technology的其它文章
- Round robin using the depth of penetration test method on an armour grade alumina
- Sonochemically assisted synthesis of nano HMX
- Effect of particle gradation of aluminum on the explosion field pressure and temperature of RDX-based explosives in vacuum and air atmosphere
- FEM analysis and experimental investigation of force and chip formation on hot turning of Inconel 625
- Study on liquid-filled structure target with shaped charge vertical penetration
- Thermal decomposition of ammonium perchlorate catalyzed with CuO nanoparticles