Experimental investigation on cenosphere-aluminum syntactic foam-filled tubes under axial impact loading
2023-11-18LiWANGBoyiZHANGJianZHANGYuexinJIANGWeiWANGGaohuiWU
Li WANG, Boyi ZHANG, Jian ZHANG, Yuexin JIANG, Wei WANG, Gaohui WU
Research Article
Experimental investigation on cenosphere-aluminum syntactic foam-filled tubes under axial impact loading
1School of Civil Engineering, Harbin Institute of Technology, Harbin 150090, China2Key Lab of Structures Dynamic Behavior and Control of the Ministry of Education, Harbin Institute of Technology, Harbin 150090, China3Center for Metal Matrix Composites Engineering Technology, Harbin Institute of Technology, Harbin 150006, China
A new syntactic foam material was prepared by screening three different average particle sizes of cenospheres (150, 200, and 300 μm) from industrial waste fly ash. Axial impact testing on syntactic foam filler and foam-filled tubes was conducted using a drop hammer test machine. The effects of parameters, such as the size of cenospheres and the impact velocity, on the mechanism of deformation, mechanical characteristics, and capacity for energy absorption of the specimen were investigated. On this basis, the differences in compressive properties exhibited by the syntactic foam-filled tubes under the two loading conditions were investigated. The results indicate that with the decrease in the average diameter of cenospheres, the initial peak crushing load and mean crushing load of foam-filled tubes increase, while the compression efficiency decreases. The specific energy absorption (SEA) of the syntactic foam-filled tube can reach 25 J/g. With the increase of impact velocity, the SEA of the specimen increases slightly. It was demonstrated that the syntactic foam-filled tube exhibits a higher effective energy absorption ratio under impact loading compared to quasi-static loading.
Cenosphere-aluminum syntactic foam; Crashworthiness; Mechanical properties; Absorption of energy
1 Introduction
Over the past decades, in the face of frequent traffic accidents, there has been much research on energy-absorbing components to prevent personal injuries. Thin-walled tubes have attracted extensive attention because of their convenient preparation and good energy absorption capacity (Xu et al., 2017; Zou et al., 2017; Sun et al., 2018; Ferdynus et al., 2019; Mansor et al., 2022; Zha et al., 2022). Significant research has been undertaken on the crushing behavior of thin-walled tubes with various cross-sections, including triangular tubes, round tubes, square tubes, and corrugated tubes (Wu et al., 2016; Zhang et al., 2018; Wang et al., 2019; Sadsighi et al., 2022; Ghahremanzadeh and Pirmohammad, 2023).
To further improve the characteristics of components for energy absorption, metallic foams (Sun et al., 2016; Liu ZF et al., 2017; Zhang et al., 2021) and polymeric foams (Yan et al., 2014; Hussein et al., 2017; Liu Q et al., 2017; Sarkabiri et al., 2017; Ghamarian and Azarakhsh, 2019) are usually inserted in thin-walled tubes as fillers. Djamaluddin et al. (2015) used non-dominated sorting genetic algorithm (NSGA-II) to optimize the design of the crashing behavior of an empty double-tube, a foam-filled empty tube, and a foam-filled double-tube under axial and oblique impact loadings. Results showed that the crashworthiness of the foam-filled double-tube was about 12% better than that of the others. Hu et al. (2018) presented an aluminum foam-filled tri-tube and noted that the outer tube's diameter and wall thickness had a strong impact on the energy absorption capacity of specimens. The research by Hu et al. (2018) showed that for the aluminum foam-filled tri-tube, the influence of the outer tube's wall thickness on the energy absorption performance of the specimen was very obvious. Abedi et al. (2018) investigated polyurethane foam-filled grooved tubes with circular cross-sections. The results showed that when the groove distance is large, the manner of deformation of the foam-filled tube tends to be the diamond mode, and when the groove distance is small, the deformation mode tends to be the concertina mode. Movahedi and Linul (2017, 2021), Linul et al. (2018), and Movahedi et al. (2018) conducted much experimental research on the compression behavior of aluminum alloy foam-filled tubes at elevated temperatures. The effect of temperature on the mechanical properties of foam-filled tubes was explored in depth. Mohammadiha and Ghariblu (2018) studied the axial dynamic energy absorption properties of a foam-filled free inversion tube. According to deformation theory, they derived analytical formulas for the instantaneous reversal load of a foam-filled tube during free inversion by applying a new theoretical model. Duarte et al. (2018) analyzed the mechanical performance of extremely thin-walled aluminum alloy in-situ foam-filled tubes and pointed out that during the preparation process, the thermal treatment of the thin-walled tubes can enhance their ductility and reduce the probability of crack formation.
Compared with traditional foam-filled tubes, the crashworthiness of syntactic foam-filled tubes needs further study. Several scholars have carried out research on the influences of the syntactic foam preparation method (Kemény et al., 2022) and loading direction (Su et al., 2019) on the compressive properties of foam-filled tubes. Movahedi et al. (2022) further discussed the deformation mode of functionally graded metal syntactic foams under high-speed impact loading. Fly ash cenosphere is a kind of common industrial waste, which is gradually being used in the preparation of composite materials (Mondal et al., 2009; Braszczyńska-Malik et al., 2017). The cenosphere-aluminum syntactic foam not only has excellent energy absorption capacity, but also has a certain bearing capacity (Doddamani et al., 2015; Manakari et al., 2016; Zhang et al., 2016; Garcia et al., 2018). Combining this material with metal tubes to prepare foam-filled tube specimens can both reduce environmental pollution and reduce the preparation cost of composite foam, and will have broad application potential.
The crushing behavior of cenosphere-aluminum syntactic foam under an axial quasi-static load has been studied (Wang et al., 2021). This paper investigates the mechanical properties of syntactic foam-filled tubes under axial low-velocity impact loading. The effects of impact load velocity and the average particle size of cenospheres on the energy absorption capacity of the specimens are analyzed. The differences in deformation modes and energy absorption ratios of syntactic foam-filled tubes under different loading conditions are indicated. The organization of this paper is as follows. Section 2 introduces the preparation of the syntactic foam, the geometric parameters of specimens, and the loading scheme of the test. The evaluation indexes of the specimen under impact loading, such as initial peak crushing load, mean crushing load, and specific energy absorption (SEA), are analyzed in Section 3. Section 4 compares the foam-filled tube's crashworthiness under impact and quasi-static loads, and conclusions are presented in Section 5.
2 Materials
2.1 Material and specimen
Pressure infiltration was employed to create the cenosphere-aluminum syntactic foam used in this test. There are three types of cenospheres (58.8% SiO2, 26.1% Al2O3) (mass fraction), with typical particle sizes of 150, 200, and 300 μm, which were obtained by screening industrial fly ash. Then, the molten 1199Al (0.005% Cu, 0.003% Fe, and 0.0025% Si (mass fraction) balanced with Al as the main alloying element) was injected into the mold with cenosphere preforms, and gradually pressurized so that the voids of preforms were filled with liquid aluminum. The preparation method of the material is shown in Fig. 1.
The thin-walled empty tube used in the experiment is 6063 aluminum alloy seamless tube with outer diameter of 20 mm, wall thickness of 1.2 mm, and height of 30 mm. The material properties of 6063 aluminum alloy (0.51% Si, 0.64% Mg, and 0.27% Fe balanced with Al as the main alloying element) were obtained through uniaxial tension test, as shown in Fig. 2a. The stress–strain () curve of 6063 aluminum alloy shows four main stages: elastic stage, yield stage, strain-hardening stage, and fracture stage. Cenosphere-aluminum syntactic foam is used as the filler, and each type of cenosphere has an average particle size of 150, 200, and 300 μm. The stress–strain curves of the three types of cenosphere-aluminum syntactic foam (150SF, 200SF, and 300SF) are shown in Fig. 2b. The stress–strain curve of syntactic foam shows typical three-stage characteristics: linear elastic stage, plastic plateau stage, and compression densification stage (Duarte et al., 2018).
Fig. 1 Preparation method of cenosphere-aluminum syntactic foam: (a) preparation flow chart; (b) preparation process diagram
The syntactic foam specimens used in the experiment are shown in Fig. 3. Fig. 4 is the diameter distribution of cenospheres. The microstructure of syntactic foam is shown in Fig. 5. In the figure, bright areas are the aluminum matrix, and dark areas are cenospheres, which maintain a complete appearance and are spread equally throughout the aluminum matrix. The geometries and dimensions of specimens are listed in Table 1. In the specimen number, AX indicates axial impact, and T1.2 indicates that the tube wall thickness is 1.2 mm. The numbers 150, 200, and 300 indicate the different types of cenosphere-aluminum syntactic foam with varying average particle sizes. The numbers 5 and 6 represent the impact velocities of 5 and 6 m/s. AX-150-6, AX-200-6, and AX-300-6 respectively represent different syntactic foam cylinder specimens, and the others are foam-filled tubes.
Fig. 2 σ-ε curves of material: (a) aluminum alloy; (b) syntactic foam
Fig. 3 Specimens used in impact test: (a) syntactic foam filler; (b) syntactic foam-filled tubes
Fig. 4 Diameter distribution of cenospheres
Fig. 5 Microstructure of syntactic foam
2.2 Experimental scheme
The axial impact experiment was conducted on the INSTRON 9250HV drop hammer test machine. The experimental set-up is shown in Fig. 6. The maximum drop height of the drop hammer is 4 m. The upper part of the testing machine is additionally provided with a spring, which can increase the initial speed of the drop hammer. The maximum impact speed of the drop hammer can reach 10 m/s. Through the built-in optical acquisition system, the test machine can obtain the displacement of the drop hammer during the entire impact process. At the same time, the acceleration sensor installed on the indenter can collect the acceleration of the drop hammer. The testing machine can be controlled in two ways: impact speed and impact energy. After determining the weight of the drop hammer, the system will automatically adjust the height of the drop hammer and the compression length of the spring. The relationship between the impact speed of the drop hammer and the initial potential energy is as follows:
wheretis the impact speed,is the initial height of the drop hammer,is the weight of the drop hammer, Δandare the compression and elastic modulus of the spring, respectively, andis the acceleration under gravity.
Fig. 6 Experimental set-up
In this experiment, the impact mass is 22.71 kg. The impact velocities are 5 and 6 m/s. Specific parameters are shown in Table 1.
3 Impact experiment results
3.1 Failure mode
3.1.1Syntactic foam filler
Fig. 7 illustrates the final shape of three syntactic foam fillers. Under the impact loading with a velocity of 6 m/s, the three kinds of filler were completely collapsed and expanded radially in a crushed shape.
Table 1 Geometric parameters of specimens
Fig. 7 Specimens after impact loading: (a) AX-150-6; (b) AX-200-6; (c) AX-300-6
3.1.2Syntactic foam-filled tubes
The foam-filled tubes also show concertina failure mode under impact loading, as shown in Fig. 8. Compared with the cenosphere-aluminum syntactic foam bearing the impact load alone, due to the restraining effect of the aluminum tube on the filler, the foam-filled tubes maintain their integrity without collapse. With the increase of impact velocity, the axial deformation of the specimen increases obviously, but the failure mode basically does not change. It is noteworthy that specimen AX-T1.2-300-5 exhibits different deformation mechanisms under impact loading. This may be due to errors in the preparation and processing of the syntactic foam, which makes the specimen have certain initial defects. Under the impact load, the folds are concentrated on one side of the specimen.
Fig. 8 Specimens after impact loading: (a) AX-T1.2-150-5; (b) AX-T1.2-200-5; (c) AX-T1.2-300-5; (d) AX-T1.2-150-6; (e) AX-T1.2-200-6; (f) AX-T1.2-300-6
Fig. 9 is a comparison between the final shape of specimen AX-T1.2-150-6 (Fig. 9a) and specimen AX-T1.2-300-6 (Fig. 9b). It was found that at the same impact velocity, the axial distortion of the foam-filled tube increases with the increase of the average particle size of cenospheres in the filler. The specimen AX-T1.2-150-6 only forms a fold in the middle, while the specimen AX-T1.2-300-6 forms a fold at the upper and lower ends. This is because part of the filler in the specimen AX-T1.2-150-6 is broken under the impact load, so that the deformation is concentrated in the middle part of the foam-filled tube. This indicates that the porosity of the syntactic foam rises as the diameter of the cenospheres in the filler grows, increasing the compression deformation capacity of the foam-filled tube.
Fig. 9 Comparison between the final shapes of specimens: (a) AX-T1.2-150-6; (b) AX-T1.2-300-6
3.2 Dynamic mechanical properties
3.2.1Load-displacement curves
The load-displacement curves of each set of specimens acquired in the experiment are shown in Fig. 10. Three kinds of syntactic foam filler exhibit typical three-stage features of elastic stage, plastic plateau stage, and densification stage under impact load (Fig. 10a). This may be because the impact resistance of the specimen is distinctly improved by the aluminum tube, so that the impact load fails to compress the specimen to the densification stage. Compared with the peak load, the load of three types of syntactic foam in the plateau stage is relatively close. In the densification stage, the load of 300SF far exceeds the load of the other two kinds of syntactic foam. This is because the porosity of 300SF is the largest and the specimen becomes the densest under the impact load.
Fig. 10 Load-displacement curves of specimens: (a) AX-6; (b) AX-T1.2-5; (c) AX-T1.2-6
The characteristics of load–displacement curves of syntactic foam-filled tubes (150SFFT, 200SFFT, 300SFFT) under two kinds of impact velocities are basically the same, but there is no densification stage in the curves (Figs. 10b and 10c). Unlike the syntactic foam that bears the impact load alone, the foam-filled tubes show obvious strength differences during the plateau stage. Of the different types of foam-filled tubes, the compression stroke of 300SFFT is the largest, while the compression stroke of 150SFFT is the smallest.
In this study, a set of parameters are proposed and compared to assess the crashworthiness of energy-absorbing materials and components under impact load (Hanssen et al., 2000; Hou et al., 2007; Guler et al., 2010; Sun et al., 2010). The relevant experimental parameters for all specimens are summarized in Table 2. The following is the definition of the energy absorption efficiency(Hanssen et al., 2000):
where() is the impact loading,is the compression stroke,maxis the maximum impact loading in the range [0,], andis the height of the specimen. As the compression stroke lengthens, so does the energy absorption efficiency. The effective compression strokeefis defined as the corresponding compression stroke when the energy absorption efficiency achieves its greatest value (Fig. 11). In the case of some load–displacement curves with no densification tendency, the effective compression stroke is taken as the entire compression stroke.
Table 2 Mechanical properties of the syntactic foam specimens
CLE: crushing load efficiency
Fig. 11 Energy absorption efficiency curve and load–displacement curve
3.2.2Peak crushing loading
The peak crushing loadingpof foam-filled tubes and syntactic foam under axial impact loading is presented in Fig. 12. The figure shows that the peak crushing loading of 150SFFT is the highest, and the peak crushing loadings of 200SFFT and 300SFFT decrease sequentially. The aluminum tube restricts the cracking and radial expansion of the filler, which enhances the peak crushing loading of the foam-filled tube.
Fig. 12 Peak crushing loading of specimens
3.2.3Mean crushing loading
The mean crushing loadingmprimarily represents the specimen's load level during the energy absorption process, which is described as (Sun et al., 2010):
The mean crushing loading of syntactic foam and foam-filled tubes under axial impact load is shown in Fig. 13. The variation trend of the mean crushing loading of specimens is basically consistent with that of the initial peak crushing load. However, the mean crushing loads of three kinds of syntactic foam filler are closer, among which the mean crushing load of 150SF is only 13.6% higher than that of 200SF. The restraining effect of the aluminum tube on the syntactic foam filler can significantly increase the mean crushing loading of the specimen. The mean crushing loading of the foam-filled tube is enhanced by 156% on average when compared to the syntactic foam filler. The increase in impact velocity has little effect on the mean crushing loading of the specimen.
Fig. 13 Mean crushing loading of specimens
3.2.4Crushing load efficiency (CLE)
The ideal energy-absorbing structure can not only fully absorb the impact energy, but also ensure the stability of the bearing capacity. CLE is an evaluation index of load consistency under impact load, defined as (Hanssen et al., 2000):
Fig. 14 plots the CLE of each specimen. When the impact velocity is 5 m/s, the CLE of the three types of foam-filled tubes varies little. When the impact velocity is 6 m/s, it can be found that the syntactic foam and foam-filled tubes gradually increase in CLE as the particle size of the cenospheres increases, which means that the initial impact effect of the specimen decreases.
Fig. 14 CLE of specimens
3.3 Capacity for energy absorption
3.3.1Effective energy absorption
The effective energy absorptionefmainly measures the energy absorption capacity of the sample in the plastic deformation stage. Its definition is as follows (Sun et al., 2010):
Fig. 15 depicts the effective energy absorption of each sample. Combined with the experimental phenomena, it can be found that the aluminum tube can restrain the deformation of the syntactic foam filler to avoid being crushed and can greatly boost the specimen's effective energy absorption. Since none of the load–displacement curves of the foam-filled tubes reaches the densification stage, the effective energy absorption of the specimen is only related to the impact velocity. Under the same impact velocity, the difference in effective energy absorption of various foam-filled tubes is not obvious.
Fig. 15 Effective energy absorption of specimens
Fig. 16 compares the load–displacement superposition curve of the syntactic foam filler (AX-150-6) and the empty aluminum tube (ET) with the load–displacement curve of specimen AX-T1.2-150-6. The shaded area is the increment of effective energy absorption caused by the interaction effect. The percentage of effective energy absorption due to the interaction effect in each specimen is shown in Fig. 17. It can be found that the interaction effect between the syntactic foam filler and the aluminum tube is gradually enhanced with the decrease of the average particle size of cenospheres under the impact load.
Fig. 16 Interaction effect of specimen AX-T1.2-150-6
Fig. 17 Percentage of effective energy absorption due to the interaction effect
3.3.2Specific energy absorption (SEA)
The SEA represents the amount of energy absorbed per unit mass of sample in the effective compression stroke, and is defined as follows (Sun et al., 2010):
where Δis the mass of the specimen. The SEA of several types of specimens under impact loading is depicted in Fig. 18. The results indicate that, as the particle size in the filler increases, the SEA of the specimen decreases. Each syntactic foam-filled tube has an SEA of over 15 J/g, of which the SEA of 150SFFT reaches 25 J/g. As shown in Fig. 19, the syntactic foam-filled tube (specimen AX-T1.2-150-6) exhibited better energy absorption capacity under low-velocity impact loading compared to the polyurethane foam-filled tube (Pirmohammad et al., 2019), aluminum foam-filled tube (Salehi et al., 2021), and zinc foam-filled tube (Salehi et al., 2021). This is because the cenospheres in the syntactic foam can absorb more energy during the process of being crushed and compacted under impact load (Zhang et al., 2016). With the increase in impact velocity, the SEA of the specimen is slightly increased.
Fig. 19 SEA of different kinds of foam-filled tubes
Fig. 18 SEA of specimens
4 Comparative analysis of foam-filled tubes under different loading
To compare the deformation failure mode, mechanical characteristics, and energy absorption performance of foam-filled tubes under impact loading and quasi-static loading, specimen AX-T1.2-150 was selected for a quasi-static compression test. The quasi-static compression test was carried out on a universal testing machine with the loading speed of 1.8 mm/min.
4.1 Comparison of deformation modes
The deformation process of the specimen AX-T1.2-150 is presented in Fig. 20. The plastic deformation of the specimen is relatively concentrated, and only one fold is generated in the middle of the specimen under the impact loading. However, under quasi-static loading, three folds are uniformly formed along the height of the specimen, indicating that the plastic deformation of the specimen is greater. At the end of the quasi-static loading process, due to the asymmetric deformation of the specimen, the wall tube is partially torn. This is mainly due to machining errors and the inhomogeneity of materials, which lead to certain initial defects in the specimen. Compared with the impact load, the loading rate of the quasi-static load is lower, which leads to more internal defect development of the material, and the tube wall cracks.
Fig. 20 Deformation mode of specimen AX-T1.2-150: (a) quasi-static loading; (b) impact loading
4.2 Comparison of mechanical characteristics and energy absorption performance
Fig. 21 shows the load–displacement curves of specimen AX-T1.2-150 under quasi-static loading and impact loading with impact velocity of 6 m/s. Table 3 is a comparison between the mechanical properties of specimen AX-T1.2-150 under two loading modes. As a result of the strain rate effect, the peak crushing load of the specimen under impact loading is 1.93 times of the quasi-static loading, and the mean crushing load also increases slightly.
To compare the energy absorption capacity of specimens under different loading modes more intuitively, the effective energy absorption ratiois calculated as follows:
Fig. 21 Load–displacement curve of specimen AX-T1.2-150 under quasi-static loading and impact loading
Table 3 Mechanical properties of specimen AX-T1.2-150 under quasi-static loading and impact loading
wheretis the total energy applied by the test instrument during loading. The energy absorption capacity of specimen AX-T1.2-150 under two loading modes is shown in Fig. 22. It can be found that the effective energy absorption ratio of the syntactic foam-filled tube under impact loading is significantly higher than that under quasi-static loading, reaching 97.8%. Cenosphere-aluminum syntactic foam exhibits a higher stress level and energy absorption capacity under impact loading and is an excellent cushioning energy absorption material.
Fig. 22 Energy absorption capacity of specimen AX-T1.2-150 under quasi-static loading and impact loading
5 Conclusions
In this study, axial impact tests were carried out on different types of cenosphere-aluminum syntactic foam-filled tubes, and the failure mode of deformation, mechanical characteristics, and energy absorption performance of specimens under impact loading were studied. The influence of parameters such as pore size in syntactic foam and impact velocity was analyzed. On this basis, the crushing characteristics of foam-filled tubes under different load conditions were compared and analyzed. The main findings include:
(1) Three kinds of syntactic foam-filled tubes buckled outwards in a concertina mode under impact loading, but the position and number of folds were different. With the increase of the pore size of syntactic foam filler, the plastic deformation capacity of the specimen increased.
(2) The aluminum tube can effectively limit the cracking of the filler, so that the initial peak crushing load and mean crushing load of the specimen were significantly improved. The increase in impact velocity had little effect on the mechanical properties of the specimen.
(3) The SEA of all cenosphere-aluminum syntactic foam-filled tubes under two impact velocities was higher than 15 J/g, and the SEA of 150SFFT reached 25 J/g, which is better than that of ordinary aluminum foam components.
(4) The peak load of 150SFFT under axial impact loading was 1.93 times that under quasi-static compression, and the mean crushing load increased slightly. The stress level of the material was increased under the impact loading, so the effective energy absorption ratio of the specimen reached 97.8%.
Acknowledgments
This work is supported by the National Natural Science Foundation of China (Nos. 51578201 and 51778196) and the Heilongjiang Provincial Natural Science Foundation of China (No. LH2020E058).
Author contributions
Boyi ZHANG and Wei WANG designed the research. Gaohui WU processed the corresponding data. Li WANG wrote the first draft of the manuscript. Jian ZHANG helped to organize the manuscript. Yuexin JIANG revised and edited the final version.
Conflict of interest
Li WANG, Boyi ZHANG, Jian ZHANG, Yuexin JIANG, Wei WANG, and Gaohui WU declare that they have no conflict of interest.
Abedi MM, Niknejad A, Liaghat GH, et al, 2018. Foam-filled grooved tubes with circular cross section under axial compression: an experimental study., 42(4):401-413. https://doi.org/10.1007/s40997-017-0106-0
Braszczyńska-Malik KN, Kamieniak J, 2017. AZ91 magnesium matrix foam composites with fly ash cenospheres fabricated by negative pressure infiltration technique., 128:209-216. https://doi.org/10.1016/j.matchar.2017.04.005
Djamaluddin F, Abdullah S, Ariffin AK, et al., 2015. Optimization of foam-filled double circular tubes under axial and oblique impact loading conditions., 87:1-11. https://doi.org/10.1016/j.tws.2014.10.015
Doddamani M, Kishore, Shunmugasamy VC, et al., 2015. Compressive and flexural properties of functionally graded fly ash cenosphere–epoxy resin syntactic foams., 36(4):685-693. https://doi.org/10.1002/pc.22987
Duarte I, Krstulović-Opara L, Vesenjak M, 2018. Axial crush behaviour of the aluminium alloy in-situ foam filled tubes with very low wall thickness., 192:184-192. https://doi.org/10.1016/j.compstruct.2018.02.094
Ferdynus M, Kotełko M, Urbaniak M, 2019. Crashworthiness performance of thin-walled prismatic tubes with corner dents under axial impact–numerical and experimental study., 144:106239. https://doi.org/10.1016/j.tws.2019.106239
Garcia CD, Shahapurkar K, Doddamani M, et al., 2018. Effect of arctic environment on flexural behavior of fly ash cenosphere reinforced epoxy syntactic foams., 151:265-273. https://doi.org/10.1016/j.compositesb.2018.06.035
Ghahremanzadeh Z, Pirmohammad S, 2023. Crashworthiness performance of square, pentagonal, and hexagonal thin-walled structures with a new sectional design., 30(12):2353-2370. https://doi.org/10.1080/15376494.2022.2053910
Ghamarian A, Azarakhsh S, 2019. Axial crushing analysis of polyurethane foam-filled combined thin-walled structures: experimental and numerical analysis., 24(6):632-644. https://doi.org/10.1080/13588265.2018.1506604
Guler MA, Cerit ME, Bayram B, et al., 2010. The effect of geometrical parameters on the energy absorption characteristics of thin-walled structures under axial impact loading., 15(4):377-390. https://doi.org/10.1080/13588260903488750
Hanssen AG, Langseth M, Hopperstad OS, 2000. Static and dynamic crushing of circular aluminium extrusions with aluminium foam filler., 24(5):475-507. https://doi.org/10.1016/S0734-743X(99)00170-0
Hou SJ, Li Q, Long SY, et al., 2007. Design optimization of regular hexagonal thin-walled columns with crashworthiness criteria., 43(6-7):555-565. https://doi.org/10.1016/j.finel.2006.12.008
Hu DY, Wang YZ, Song B, et al., 2018. Energy absorption characteristics of a foam-filled tri-tube under axial quasi-static loading: experiment and numerical simulation., 23(4):417-432. https://doi.org/10.1080/13588265.2017.1331494
Hussein RD, Ruan D, Lu GX, et al., 2017. Crushing response of square aluminium tubes filled with polyurethane foam and aluminium honeycomb., 110:140-154. https://doi.org/10.1016/j.tws.2016.10.023
Kemény A, Movahedi N, Fiedler T, et al., 2022. The influence of infiltration casting technique on properties of metal syntactic foams and their foam-filled tube structures., 852:143706. https://doi.org/10.1016/j.msea.2022.143706
Linul E, Movahedi N, Marsavina L, 2018. The temperature and anisotropy effect on compressive behavior of cylindrical closed-cell aluminum-alloy foams., 740:1172-1179. https://doi.org/10.1016/j.jallcom.2018.01.102
Liu Q, Fu J, Wang JS, et al., 2017. Axial and lateral crushing responses of aluminum honeycombs filled with EPP foam., 130:236-247. https://doi.org/10.1016/j.compositesb.2017.07.041
Liu ZF, Huang ZC, Qin QH, 2017. Experimental and theoretical investigations on lateral crushing of aluminum foam-filled circular tubes., 175:19-27. https://doi.org/10.1016/j.compstruct.2017.05.004
Manakari V, Parande G, Gupta M, 2016. Effects of hollow fly-ash particles on the properties of magnesium matrix syntactic foams: a review., 5(1):116-131. https://doi.org/10.1520/MPC20150060
Mansor MA, Ahmad Z, Abdullah MR, 2022. Crashworthiness capability of thin-walled fibre metal laminate tubes under axial crushing., 252:113660. https://doi.org/10.1016/j.engstruct.2021.113660
Mohammadiha O, Ghariblu H, 2018. Crashworthiness study and optimisation of free inversion foam-filled tubes under dynamic loading., 23(6):605-617. https://doi.org/10.1080/13588265.2017.1368119
Mondal DP, Das S, Ramakrishnan N, et al., 2009. Cenosphere filled aluminum syntactic foam made through stir-casting technique., 40(3):279-288. https://doi.org/10.1016/j.compositesa.2008.12.006
Movahedi N, Linul E, 2017. Quasi-static compressive behavior of the ex-situ aluminum-alloy foam-filled tubes under elevated temperature conditions., 206:182-184. https://doi.org/10.1016/j.matlet.2017.07.018
Movahedi N, Linul E, 2021. Radial crushing response of ex-situ foam-filled tubes at elevated temperatures., 277:114634. https://doi.org/10.1016/j.compstruct.2021.114634
Movahedi N, Linul E, Marsavina L, 2018. The temperature effect on the compressive behavior of closed-cell aluminum-alloy foams., 27(1):99-108. https://doi.org/10.1007/s11665-017-3098-4
Movahedi N, Fiedler T, Taşdemirci A, et al., 2022. Impact loading of functionally graded metal syntactic foams., 839:142831. https://doi.org/10.1016/j.msea.2022.142831
Pirmohammad S, Ahmadi-Saravani S, Zakavi SJ, 2019. Crashworthiness optimization design of foam-filled tapered decagonal structures subjected to axial and oblique impacts., 26(10):2729-2745. https://doi.org/10.1007/s11771-019-4209-1
Sadighi A, Azimi MB, Asgari M, et al., 2022. Crashworthiness of hybrid composite-metal tubes with lateral corrugations in axial and oblique loadings., 27(6):1813-1829. https://doi.org/10.1080/13588265.2021.2017654
Salehi M, Mirbagheri SMH, Ramiani AJ, 2021. Efficient energy absorption of functionally-graded metallic foam-filled tubes under impact loading., 31(1):92-110. https://doi.org/10.1016/S1003-6326(20)65480-2
Sarkabiri B, Jahan A, Rezvani MJ, 2017. Crashworthiness multi-objective optimization of the thin-walled grooved conical tubes filled with polyurethane foam., 39(7):2721-2734. https://doi.org/10.1007/s40430-017-0747-3
Su MM, Wang H, Hao H, 2019. Axial and radial compressive properties of alumina-aluminum matrix syntactic foam filled thin-walled tubes., 226:111197. https://doi.org/10.1016/j.compstruct.2019.111197
Sun GY, Li GY, Hou SJ, et al., 2010. Crashworthiness design for functionally graded foam-filled thin-walled structures., 527(7-8):1911-1919. https://doi.org/10.1016/j.msea.2009.11.022
Sun GY, Li SF, Liu Q, et al., 2016. Experimental study on crashworthiness of empty/aluminum foam/honeycomb-filled CFRP tubes., 152:969-993. https://doi.org/10.1016/j.compstruct.2016.06.019
Sun GY, Li SF, Li GY, et al., 2018. On crashing behaviors of aluminium/CFRP tubes subjected to axial and oblique loading: an experimental study., 145:47-56. https://doi.org/10.1016/j.compositesb.2018.02.001
Wang L, Zhang BY, Zhang J, et al., 2021. Deformation and energy absorption properties of cenosphere-aluminum syntactic foam-filled tubes under axial compression., 160:107364. https://doi.org/10.1016/j.tws.2020.107364
Wang Z, Jin XH, Li Q, et al., 2019. On crashworthiness design of hybrid metal-composite structures., 171:105380. https://doi.org/10.1016/j.ijmecsci.2019.105380
Wu SY, Li GY, Sun GY, et al., 2016. Crashworthiness analysis and optimization of sinusoidal corrugation tube., 105:121-134. https://doi.org/10.1016/j.tws.2016.03.029
Xu BY, Sun GY, Wu S, et al., 2017. Crashworthiness analysis and optimization of Fourier varying section tubes., 92:41-58. https://doi.org/10.1016/j.ijnonlinmec.2017.03.001
Yan LB, Chouw N, Jayaraman K, 2014. Lateral crushing of empty and polyurethane-foam filled natural flax fabric reinforced epoxy composite tubes., 63:15-26. https://doi.org/10.1016/j.compositesb.2014.03.013
Zha YB, Wang S, Ma QH, et al., 2022. Study on the axial impact of Al-CFRP thin-walled tubes with induced design., 43(7):4660-4686. https://doi.org/10.1002/pc.26720
Zhang BY, Lin YF, Li S, et al., 2016. Quasi-static and high strain rates compressive behavior of aluminum matrix syntactic foams., 98:288-296. https://doi.org/10.1016/j.compositesb.2016.05.034
Zhang BY, Zhang J, Wang L, et al., 2021. Bending behavior of cenosphere aluminum matrix syntactic foam-filled circular tubes., 243:112650. https://doi.org/10.1016/j.engstruct.2021.112650
Zhang ZY, Sun W, Zhao YS, et al., 2018. Crashworthiness of different composite tubes by experiments and simulations., 143:86-95. https://doi.org/10.1016/j.compositesb.2018.01.021
Zou X, Gao GJ, Dong HP, et al., 2017. Crashworthiness analysis and structural optimisation of multi-cell square tubes under axial and oblique loads., 22(2):129-147. https://doi.org/10.1080/13588265.2016.1235109
题目:轴向冲击载荷作用下铝基复合泡沫填充管的实验研究
作者:王理1,2,张博一1,2,张箭1,2,蒋月新1,2,王伟1,2,武高辉3
机构:1哈尔滨工业大学,土木工程学院,中国哈尔滨,150090;2哈尔滨工业大学,结构工程灾变与控制教育部重点实验室,中国哈尔滨,150090;3哈尔滨工业大学,金属基复合材料工程技术中心,中国哈尔滨,150006
目的:本文旨在分析铝基复合泡沫在轴向冲击荷载作用下不同参数(泡沫芯材平均粒径和冲击速度等)对填充管力学性能和吸能能力的影响,并研究填充管试件的设计方法,以提高泡沫填充管试件的耐撞性。
创新点:1. 利用三种新型铝基复合泡沫材料与铝管结合,制备具有优异性能的铝基复合泡沫填充管试件;2. 对比分析复合泡沫填充管在不同类型荷载作用下的吸能表现。
方法:1. 通过冲击加载实验,研究轴向冲击荷载作用下复合泡沫平均粒径和加载速度对填充管试件力学性能的影响(图12和13);2. 通过结合静力加载实验,对比分析填充管在两种荷载作用下变形模式和吸能能力的特点,并验证复合泡沫填充管缓冲吸能的优越性(图22)。
结论:1. 随着复合泡沫芯材平均孔径的增加,试件的塑性变形能力增强。2. 铝管能有效限制芯材的开裂,使试件的初始峰值压碎载荷和平均压碎载荷均有明显提高。3. 所有铝复合泡沫填充管在冲击加载下的比吸能均高于15 J/g;其中150SFFT的比吸能可达25 J/g,优于普通泡沫铝试件。4. 150SFFT在轴向冲击载荷下的峰值载荷是静态压缩载荷下的1.93倍;冲击载荷下材料的应力水平提高,且填充管试件的有效吸能率可达97.8%。
关键词:铝基复合泡沫;耐撞性;力学性能;能量吸收
https://doi.org/10.1631/jzus.A2200430
https://doi.org/10.1631/jzus.A2200430
© Zhejiang University Press 2023
Sept. 15, 2022;
Jan. 21, 2023;
July 22, 2023; Online first Sept. 8, 2023
猜你喜欢
杂志排行
Journal of Zhejiang University-Science A(Applied Physics & Engineering)的其它文章
- Core-drilling kinematic modeling and analysis of Jiaolong submersible manipulator
- Effect of carbon dioxide concentration on the combustion characteristics of boron agglomerates in oxygen-containing atmospheres
- Short-term tunnel-settlement prediction based on Bayesian wavelet: a probability analysis method
- Correlation between travel experiences and post-COVID outbound tourism intention: a case study from China
- Advances in micro-nano biosensing platforms for intracellular electrophysiology
- Biomaterial types, properties, medical applications, and other factors: a recent review